| GRADE | Werks Toff | UNS | Ni | Cr | Co | Mo | Fe | Cu | Nb | Al | Ti | C | S | Si | Mn | others | Tensile Strength Rm (Mpa) | Yield strength Rp0.2 (Mpa) | Elongation A% | Density (g/cm3) |
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Hastelloy X | 2.4665 | N06002 | Remainder | 20.5 - 23.0 | 0.50 - 2.5 | 8.0 - 10.0 | 17-20 | 0.50 Max | - | 0.50 Max | 0.15 Max | 0.05-0.15 | 0.03 Max | 1.00 Max | 1.00 Max | P-0.04 Max / W-0.2-1 / B-0.008 Max |
755 | 385 | 49.50 | 8.22 |
| Hastelloy B2 | 2.4617 | N10665 | 69.00 | 1.00 | 1.00 | 28.00 | 2.00 | - | - | - | - | 0.01 | - | 0.10 | 1.00 | - | 914 | 396 | 40 | 9.22 |
| Hastelloy C22 | 2.4602 | N06022 | Remainder | 20.0 - 22.5 | 2.5 Min | 12.5 - 14.5 | 2.0 - 6.0 | - | - | - | - | 0.015 Max | 0.02 Max | 0.08 Max | 0.50 Max | W - 2.5-3.5 / V - 0.35 Min / P - 0.02 Max |
690 | 310 | 45 | 8.69 |
| Hastelloy C276 | 2.4819 | N10276 | 57.00 | 14.5 -16.5 | 2.50 | 15.0 - 17.0 | 4.0 - 7.0 | - | - | - | - | 0.01 | 0.01 | 0.08 | 1.00 | W - 3 - 4.5 / V - 0.35 / P - 0.025 |
690 | 285 | 40 | 8.89 |
| Inconel 718 | 2.4668 | N07718 | 50.0 -55.0 | 17.0 - 21.0 | 1.00 Max | 2.80 - 3.30 | Bal | 0.30 Max | 4.75 - 5.50 | 0.20-0.80 | 0.65-1.15 | 0.08 Max | 0.015 Max | 0.35 Max | 0.35 Max | P - 0.015 Max / B - 0.006 Max / Ta - 0.05 Max |
1240 | 1034 | 30 | 8.19 |
| Inconel 600 | 2.4816 | N06600 | 72.00 | 14.0 - 17.0 | - | - | 6.0 - 10.0 | 0.50 Max | - | 0.30 Max | 0.3 Max | 0.05 - 0.15 | 0.015 Max | 0.50 Max | 1.00 Max | B - 0.006 Max / P - 0.015 Max |
620 | 275 | 30 | 8.47 |
| Inconel 601 | 2.4851 | N06601 | 58.0 - 63.0 | 21.0 - 25.0 | - | - | Bal | 1.00 Max | - | 1.0 -1.7 | - | 0.1 Max | 0.015 Max | 0.50 Max | 1.00 Max | - | 550 | 205 | 30 | 8.11 |
| Inconel 625 | 2.4856 2.4831 | N06625 | 58.00 Min | 20.0 - 23.0 | 1.00 Max | 8.0 - 10.0 | 5.00 Max | - | 3.15 - 4.15 | 0.40 Max | 0.4 Max | 0.10 Max | 0.015 Max | 0.50 Max | 0.50 Max | P - 0.015 Max | 827 | 414 | 40 | 8.44 |
| Inconel 800 | 1.4876 | N08800 | 30.0 - 35.0 | 19.0 - 23.0 | - | - | 39.5 Min | 0.75 Max | - | 0.15 - 0.60 | 0.15 - 0.60 | 0.10 Max | 0.01 Max | 1.00 Max | 1.50 Max | - | 515 | 210 | 30 | 7.94 |
| Inconel 825 | 2.4858 | N08825 | 38.0 - 46.0 | 19.5 - 23.5 | - | 2.5 - 3.5 | 22.0 Min | 1.5 - 3.0 | - | 0.20 Max | 0.6 - 1.2 | 0.05 Max | 0.03 Max | 0.50 Max | 1.00 Max | - | 586 | 241 | 30 | 8.14 |
| Inconel X-750 | 2.4669 | N07750 | 70.00 Min | 14.0 - 17.0 | 1.00 Max | - | 5.0 - 9.0 | 0.50 Max | 0.70 - 1.20 | 0.40 - 1.0 | 2.25 - 2.75 | 0.08 Max | 0.01 Max | 0.50 Max | 1.00 Max | - | 1200 | 820 | 30 | 8.28 |
| Monel 400 | 2.4360 | N04400 | 63.00 Min | - | - | - | 2.5 Max | 28.0 - 34.0 | - | - | - | 0.30 Max | 0.024 Max | 0.50 Max | 2.0 Max | - | 550 | 275 | 30 | 8.80 |
| Monel K-500 | 2.4375 | N05500 | 63.00 Min | - | - | - | 2.0 Max | 27.0 - 33.0 | - | 2.30 - 3.15 | 0.35 - 0.85 | 0.25 Max | 0.01 Max | 0.50 Max | 1.5 Max | - | 1000 | 655 | 40 | 8.44 |
| Alloy L-605 | 2.4964 | R30605 | 9.0 - 11.0 | 19.0 - 21.0 | Bal | - | 3.0 Max | - | - | - | - | 0.05 - 0.15 | 0.03 Max | 0.40 Max | 1.0 - 2.0 | P - 0.04 Max / W - 14.0 - 16.0 | 600 | 275 | 30 | 9.13344 |
| Nickel 200 | 2.4066 2.4060 | N02200 | 99.00 Min | - | - | - | 0.40 Max | 0.25 Max | - | - | - | 0.15 Max | 0.010 Max | 0.35 Max | 0.35 Max | - | 415 | 105 | 35 | 8.89 |
| Alloy 20 | 2.4660 | N08020 | 32.0 - 38.0 | 19.0 - 21.0 | - | 2.0 - 3.0 | Bal | 3.0 - 4.0 | 1.00 Max | - | - | 0.07 Max | 0.035 Max | 1.0 Max | 2.00 Max | P - 0.045 Max | 655 | 240 | 35 | 8.1 |
| Nimonic 80A | 2.4952 2.4631 | N07080 | Bal | 18.0 - 21.0 | 2.0 Max | - | 3.0 Max | 0.20 Max | - | 1.0 - 1.8 | 1.8 - 2.7 | 0.10 Max | 0.015 Max | 1.0 Max | 1.00 Max | B - 0.008 Max / Zr - 0.15 Max |
1100 | 650 | 30 | 8.19 |
| 904L | 1.4539 | N08904 | 23.0 - 28.0 | 19.0 - 23.0 | - | 4.0 - 5.0 | Bal | 1.0 - 2.0 | - | - | - | 0.02 Max | 0.035 Max | 1.0 Max | 2.00 Max | P - 0.045 Max | 490 | 220 | 35 | 7.95 |
| Duplex 2205 | 1.4462 | S32205 | 4.5 - 6.5 | 22.0 - 23.0 | - | 3.0 - 3.5 | Bal | - | - | - | - | 0.03 Max | 0.02 Max | 1.00 Max | 2.00 Max | P - 0.030 Max / N - 0.14 - 0.20 |
620 | 450 | 25 | 7.8 |
| Super Duplex 32750 | 1.4410 | S32750 | 6.0 - 8.0 | 24.0 - 26.0 | - | 3.0 - 3.5 | Bal | 0.50 Max | - | - | - | 0.03 Max | 0.02 Max | 0.80 Max | 1.20 Max | P - 0.035 Max / N - 0.24 - 0.32 |
800 | 550 | 25 | 7.8 |
| SMO 254 | 1.4547 | S31254 | 17.5 - 18.5 | 19.5 - 20.5 | - | 6.0 - 6.5 | - | 0.5 - 1.0 | - | - | - | 0.02 Max | 0.01 Max | 0.7 Max | 1.00 Max | P - 0.03 Max / N - 0.18 - 0.22 |
650 | 280 | 40 | 8 |
Disclaimer: Inconel, Monel, Hastelloy are registered trademark of Specific manufacturer, name are listed for reference to helpo identity of the grade.