| Hastelloy X |
2.4665 |
N06002 |
Remainder |
20.5-23 |
0.5-2.5 |
8-10 |
17-20 |
0.5 Max |
- |
0.5 Max |
0.15 Max |
0.05-0.15 |
0.03 Max |
1 Max |
1 Max |
W-0.2-1.0 Max/V-0.2-0.4/B-0.008 Max |
765 |
385 |
45-50% |
8.22 |
| Hastelloy B2 |
2.4617 |
N10665 |
69 |
1 |
1 |
28 |
2 |
- |
- |
- |
- |
0.01 |
- |
0.1 |
1 |
|
874 |
396 |
40% |
9.22 |
| Hastelloy C22 |
2.4602 |
N06022 |
Remainder |
20-22.5 |
2.5 Max |
12.5-14.5 |
2-6 |
- |
- |
- |
- |
0.015 Max |
0.02 Max |
0.08 Max |
0.5 Max |
W-2.5-3.5/V-0.35 Max/P-0.02 Max |
690 |
310 |
45 |
8.69 |
| Hastelloy C276 |
2.4819 |
N10276 |
57.00 |
14.5-16.5 |
2.50 |
15-17 |
4-7 |
- |
- |
- |
- |
0.01 |
0.01 |
0.08 |
1 |
W-3-4.5/V-0.35/P-0.04 Max |
690 |
285 |
40 |
8.89 |
| Inconel 718 |
2.4668 |
N07718 |
50.0-55.0 |
17.0-21.0 |
1.00 Max |
2.80-3.30 |
Bal |
0.30 Max |
4.75-5.50 |
0.30-0.80 |
0.65-1.15 |
0.08 Max |
0.015 Max |
0.35 Max |
0.35 Max |
B-0.006 Max/P-0.015 Max/Ta-0.05 Max |
1240 |
1034 |
25 |
8.19 |
| Inconel 600 |
2.4816 |
N06600 |
72.00 |
14.0-17.0 |
- |
- |
6.0-10.0 |
0.5 Max |
- |
0.3 Max |
0.3 Max |
0.05-0.10 |
0.015 Max |
0.5 Max |
1.0 Max |
P-0.015 Max/Cu-0.5 Max |
550 |
240 |
30 |
8.47 |
| Inconel 601 |
2.4851 |
N06601 |
58.0-63.0 |
21.0-25.0 |
- |
- |
Bal |
1 Max |
- |
1.0-1.7 |
- |
0.1 Max |
0.015 Max |
0.5 Max |
1.0 Max |
|
550 |
205 |
30 |
8.17 |
| Inconel 625 |
2.4856 |
N06625 |
58.00 Min |
20-23 |
1 Max |
8-10 |
5 Max |
- |
3.15-4.15 |
0.4 Max |
0.4 Max |
0.10 Max |
0.015 Max |
0.5 Max |
0.5 Max |
P-0.015 Max |
827 |
414 |
40 |
8.44 |
| Inconel 800 |
1.4876 |
N08800 |
30 - 35 |
19 - 23 |
- |
- |
39.5 Min |
0.75 Max |
- |
0.15 - 0.60 |
0.15 - 0.60 |
0.10 Max |
0.01 Max |
1.00 Max |
1.5 Max |
- |
515 |
210 |
30 |
7.94 |
| Inconel 825 |
2.4858 |
N08825 |
38 - 46 |
19.5 - 23.5 |
- |
2.5 - 3.5 |
22.0 Min |
1.5 - 3.0 |
- |
0.2 Max |
0.6 - 1.2 |
0.05 Max |
0.03 Max |
0.5 Max |
1.0 Max |
- |
586 |
241 |
30 |
8.14 |
| Inconel X-750 |
2.4669 |
N07750 |
70.00 Min |
14.0-17.0 |
1.00 Max |
- |
5.0-9.0 |
0.5 Max |
0.70-1.20 |
0.40-1.0 |
2.25-2.75 |
0.08 Max |
0.01 Max |
0.50 Max |
1.00 Max |
|
- |
- |
- |
8.28 |
| Monel 400 |
2.4360 |
N04400 |
63.0-70.0 |
- |
- |
- |
2.5 Max |
Bal |
- |
- |
- |
0.3 Max |
0.024 Max |
0.5 Max |
2.0 Max |
|
550 |
275 |
30 |
8.80 |
| Monel K-500 |
2.4375 |
N05500 |
63.00 Min |
- |
- |
- |
2.0 Max |
27.0-33.0 |
- |
2.30-3.15 |
0.35-0.85 |
0.25 Max |
0.01 Max |
0.5 Max |
1.5 Max |
|
- |
- |
- |
8.44 |
| Alloy L-605 |
2.4964 |
R30605 |
9.0 -11.0 |
19.0-21.0 |
Bal |
- |
3.0 Max |
- |
- |
- |
- |
0.05-0.15 |
0.03 Max |
0.40 Max |
1.0-2.0 |
W-14-16 Max/P-0.04 Max |
- |
- |
- |
9.13-9.24 |
| Nickel 200 |
2.4060 |
N02200 |
99.00 Min |
- |
- |
- |
0.40 Max |
0.25 Max |
- |
- |
- |
0.15 Max |
0.01 Max |
0.35 Max |
0.35 Max |
|
475 |
185 |
35 |
8.89 |
| Nickel 201 |
2.4061 |
N02201 |
99.00 Min |
- |
- |
- |
0.40 Max |
0.25 Max |
- |
- |
- |
0.02 Max |
0.01 Max |
0.35 Max |
0.35 Max |
|
410 |
205 |
35 |
8.89 |
| Nimonic 80A |
2.4952/2.4631 |
N07080 |
Bal |
18.0-21.0 |
2.0 Max |
- |
3.0 Max |
0.2 Max |
- |
1.0-1.8 |
1.8-2.7 |
0.10 Max |
- |
1.0 Max |
1.2 Max |
B-0.008 Max/Zr-0.15 Max |
- |
- |
- |
8.19 |
| 904L |
1.4539 |
N08904 |
23 -28 |
19 -23 |
- |
4 -5 |
Bal |
1 -2 |
- |
- |
- |
0.02 Max |
0.035 Max |
1.0 Max |
2.0 Max |
P-0.045 Max |
- |
- |
- |
7.95 |
| Duplex 2205 |
1.4462 |
S32205 |
4.5-6.5 |
22.0-23.0 |
- |
3.0-3.5 |
Bal |
0.5 Max |
- |
- |
- |
0.03 Max |
0.02 Max |
1.00 Max |
2.0 Max |
P-0.03 Max/N-0.14-0.20 |
620 |
450 |
- |
7.8 |
| Super Duplex S32750 |
1.4410 |
S32750 |
6.0 -8.0 |
24.0 -26.0 |
- |
3.0-3.5 |
Bal |
0.5 Max |
- |
- |
- |
0.03 Max |
0.02 Max |
0.80 Max |
1.20 Max |
P-0.035 Max/N-0.24-0.32 |
- |
- |
- |
7.8 |
| SMO 254 |
1.4547 |
S31254 |
17.5 -18.5 |
19.5 -20.5 |
- |
6.0 -6.5 |
- |
0.5-1.0 |
- |
- |
- |
0.02 Max |
0.01 Max |
0.8 Max |
1.0 Max |
P-0.03 Max/N-0.18-0.22 |
- |
- |
- |
8 |